Glass Transition Temperatures (K)
Poly(1,4-biphenyl ether ether sulfone), PPSU | 482 |
PoIy(1,2-butadiene) | 261 |
Poly(1,4-butadiene) | 168 |
Poly(1,4-butane sebacate) | 214 |
Poly(1-butene) | 244 |
Poly(1,4-butylene adipate) | 205 |
Poly(1-chloromethyl)ethylene oxide) | 250 |
Poly(1,4-cyclohexanecarbonate) | 400 |
Poly(1-(diethylamino)ethyl methacrylate) | 293 |
Poly(1-(dimethylamino)ethyl methacrylate) | 292 |
Poly(1,2-ethylene carbonate) | 290 |
Poly(1,6-hexylene carbonate) | 271 |
Poly(1-methyl-1-butenylene) | 203 |
Poly(1-octene) | 218 |
Poly(1,8-octylene carbonate) | 266 |
Poly(1-pentene) | 238 |
PoIy(1-pentenylene) | 176 |
Poly(1,5-pentylene carbonate) | 277 |
Poly(1,4-phenyl ether), PPE | 361 |
Poly(1,4-phenylene ether ether sulfone), PEE | 479 |
Poly(1,4-phenylene ether-sulfone), PES | 490 |
Poly(1,4-phenylene sulfide), PPS | 363 |
Poly(1,2-propylene carbonate) , PPC | 310 |
Poly[1-(tert-butyl)ethene] | 337 |
Poly(2-chloro-p-xylylene) | 356 |
Poly(2-chlorostyrene) | 395 |
Poly(2-cyanobutyl acrylate) | 384 |
Poly(2-cyanoethyl acrylate) | 277 |
Poly(2,6-dimethyl-p-phenylene oxide), PPO | 487 |
Poly(2,6-diphenyl-p-phenylene oxide) | 497 |
Poly(2-ethyl-2-methylpropylene terephthalate) | 328 |
Poly(2-ethylhexyl acrylate) | 221 |
Poly(2-hydroxyethyl methacrylate), PHEMA | 350 |
Poly(2-hydroxypropyl methacrylate) | 345 |
Poly(2-methoxystyrene) | 348 |
Poly(2-methylstyrene) | 409 |
Poly(2-phenylethyl methacrylate) | 299 |
Poly(2,2,3,3-tetrafluoropropyl acrylate) | 249 |
Poly(2,2,3,3-tetrafluoropropyl methacrylate) | 344 |
Poly(2,6,3',5'-tetrachloro bisphenol A carbonate) | 500 |
Poly(2,2,2-trifluoroethyl methacrylate) | 347 |
Poly(3-hexoxypropylene oxide) | 189 |
Poly(3-methylstyrene) | 370 |
Poly(3,3'-oxydiphenylene carbonate) | 364 |
Poly(3,3,5-trimethylcyclohexyl acrylate) | 302 |
Poly(4-bromostyrene) | 411 |
Poly(4-chlorophenyl vinyl ketone) | 336 |
Poly(4-chlorostyrene) | 398 |
Poly(4-cyanobutyl acrylate) | 236 |
Poly(4,4'-dichlorobenzophenone), PEK | 428 |
Poly(4-ethylstyrene) | 326 |
Poly(4-fluorostyrene) | 376 |
Poly(4-hydroxystyrene), PVAc, PVA | 430 |
Poly(4-isopropylstyrene) | 360 |
Poly(4-methoxy-2-methylstyrene) | 361 |
Poly(4-methoxystyrene) | 386 |
Poly(4,4'-methylenedioxy dibenzoic anhydride) | 407 |
Poly(4-methylpent-1-ene) | 302 |
Poly(4-methylstyrene) | 377 |
Poly(4,4'-pentamethylenedibenzoic anhydride) | 320 |
Poly(4-phenylstyrene) | 423 |
Poly(4-tert-butylcyclohexyl methacrylate) | 403 |
Poly(4-tert-butylstyrene) | 402 |
Poly(4,4'-tetramethylenedibenzoic anhydride) | 316 |
Poly(4,4'-thiodiphenylene carbonate) | 391 |
Poly(8-aminooctanoic acid), Nylon 8 | 323 |
Polyacetal, Poly(methylene oxide), POM | 207 |
Poly(acrylamide) | 438 |
Poly(acrylic acid), PAA | 374 |
Poly(acrylonitrile), PAN | 383 |
Poly(benzyl acrylate) | 277 |
Poly(benzyl methacrylate) | 328 |
Poly{[bis(4-chlorophenyl)sulfone]-alt-[bisphenol-A]}, PSU | 457 |
Poly(Bisphenol A carbonate) | 424 |
Poly(Bisphenol A terephthalate) | 385 |
Poly(Bisphenol AP carbonate) | 460 |
Poly(bisphenol AP isophthalate) | 473 |
Poly(Bisphenol B carbonate) | 415 |
Poly(Bisphenol C carbonate) | 381 |
Poly(Bisphenol C terephthalate) | 445 |
Poly(Bisphenol E carbonate) | 416 |
Poly(Bisphenol F carbonate) | 407 |
Poly(bisphenol S-alt-terephthalic acid) | 519 |
Poly(butyl acrylate) | 220 |
Poly(butyl cyanoacrylate) | 379 |
Poly(butyl methacrylate) | 293 |
Poly(butyl vinyl ether) | 219 |
Poly(butyl vinyl thioether) | 253 |
Poly(caprolactam), Nylon 6 | 324 |
Poly(caprolactone) | 207 |
Polychloroprene, Neoprene | 237 |
Poly(chlorotrifluoroethylene) | 360 |
Poly(cyanomethyl acrylate) | 296 |
Poly(cyclohexyl acrylate) | 288 |
Poly(cyclohexyl methacrylate) | 389 |
Poly(cyclohexylethene) | 393 |
Poly(decamethylene terephthalate) | 283 |
Poly(decyl methacrylate) | 211 |
Poly(diethyl fumarate) | 284 |
Poly(diisobutyl Bisphenol A terephthalate) | 373 |
Poly(diisopropyl Bisphenol A terephthalate) | 408 |
Poly(dimethyl fumarate) | 373 |
Poly(dimethyl itaconate), PDMI | 373 |
Poly[di(n-propyl) itaconate] | 306 |
Poly(dipropyl fumarate) | 259 |
Poly(dodecyl acrylate) | 255 |
Poly(dodecyl methacrylate) | 218 |
Poly(epichlorohydrin) | 251 |
Poly(ether ketone ketone), PEKK | 437 |
Poly(ethyl acrylate) | 250 |
Poly(ethyl cyanoacrylate) | 422 |
Poly(ethyl methacrylate), PEMA | 338 |
Poly(ethyl vinyl ether) | 232 |
Poly(ethyl vinyl thioether) | 266 |
Poly(ethylene 2,6-naphthalate) | 392 |
Poly(ethylene adipate) | 230 |
Poly(ethylene glycol), PEG | 207 |
Poly[(ethylene
glycol)-alt-(hexamethylene diisocyanate)], PEG 50 - HMDI |
301 |
Poly{(ethylene
glycol)-alt-[bis(4-isocyanatophenyl)methane]}, PEG 50 - MDI |
412 |
Poly(ethylene phthalate) | 297 |
Poly(ethylene sulfide) | 223 |
Poly(ethylene terephthalate) | 346 |
Poly(ethylene) | 193 |
Poly(ethyleneketone), PEK | 288 |
Polyglycolide, PGL | 312 |
Poly(glycidyl methacrylate) | 334 |
Poly(heptane-1,7-diyl teraphthalamide) | 390 |
Poly(hexadecyl methacrylate) | 289 |
Poly(hexamethylene adipamide), Nylon 6,6 | 324 |
Poly(hexamethylene sebacamide), Nylon 6,10 | 320 |
Poly(hexamethylene terephthalate) | 291 |
Poly(hexyl acrylate) | 215 |
Poly(hexyl methacrylate) | 268 |
Poly(hexyl vinyl ether) | 198 |
Poly[(hydroquinone)-alt-(4,4'-dichlorobenzophenone)], PEEK | 420 |
Poly{hydroquinone-alt-[1,4-bis(4-fluorobenzoyl)benzene]}, PEEKK | 433 |
Poly(iminoadipoyliminoheptamethylene), Nylon 7,6 | 326 |
Poly(iminosebacoyliminodecamethylene), Nylon 10,10 | 326 |
Poly(isobornyl acrylate) | 359 |
Poly(isobornyl methacrylate) | 383 |
Poly(isobutene) | 203 |
Poly(isobutyl acrylate) | 240 |
Poly(isobutyl methacrylate) | 330 |
Poly(isobutyl vinyl ether) | 255 |
Poly(isodecyl methacrylate) | 232 |
Poly(isophthalic anhydride) | 385 |
Poly(isopropyl acrylate) | 271 |
Poly(isopropyl methacrylate) | 356 |
Poly(isopropyl vinyl ether) | 270 |
Polylactic acid, PLA | 332 |
Poly(methacrylic acid), PMAA | 501 |
Poly(methacrylonitrile) | 388 |
Poly(methyl acrylate), PMA | 283 |
Poly(methyl cyanoacrylate) | 436 |
Poly(methyl isopropenyl ketone) | 370 |
Poly(methyl methacrylate), PMMA | 378 |
Poly(methyl vinyl ether) | 245 |
Poly(methyl vinyl thioether) | 272 |
Poly(m-phenylene terephthalamide), Nomex MPDI | 537 |
Poly(N,N-dimethylacrylamide) | 379 |
Poly(neopentyl glycol succinate) | 257 |
Poly(neopentyl methacrylate) | 299 |
Poly(nonamethylene terephthalate) | 289 |
Poly(nonyl acrylate) | 200 |
Poly(norbornene) | 316 |
Poly(octadecyl acrylate) | 314 |
Poly(octadecyl methacrylate) | 311 |
Poly(octyl methacrylate) | 228 |
Poly(octyl vinyl ether) | 193 |
Poly(pentyl methacrylate) | 276 |
Poly(phenoxyethyl acrylate) | 279 |
Poly(phenyl methacrylate) | 383 |
Poly(phenyl vinyl ketone) | 323 |
Poly(p-phenylene terephthalamide), Kevlar, PPTA | 600 |
Poly(p-phenylene), PPP | 538 |
poly[(prop-1-ene)-alt-(carbon monooxide)] | 312 |
Poly(propyl acrylate) | 231 |
Poly(propyl methacrylate) | 316 |
Poly(propyl vinyl ether) | 224 |
Poly(propylene glycol), PPG | 200 |
Poly(propylene sulfide), PPS | 227 |
Poly(propylene) | 263 |
Poly(p-xylene) | 343 |
Poly-(R)-3-hydroxybutyrate | 273 |
Poly(sec-butyl acrylate) | 253 |
Polystyrene, PS | 373 |
Poly(tert-butyl acrylate) | 311 |
Poly(tert-butyl methacrylate) | 388 |
Poly(tetrachloro Bisphenol A terephthalate) | 483 |
Poly(tetradecyl methacrylate) | 264 |
Poly(tetrafluoro ethylene), Teflon, PTFE | 392 |
Poly(tetrahydro furfuryl acrylate) | 260 |
Poly(tetrahydrofuran), PTHF, PTMG | 187 |
Poly(tetrahydrofurfuryl methacrylate) | 327 |
Poly(tetramethyl bisphenol A carbonate) | 467 |
Poly(tetramethyl bisphenol A terephthalate) | 492 |
Poly[(tetramethylene isophthalate) | 297 |
Poly[(tetramethylene terephthalate) | 313 |
Poly(trifluoromethoxy 1,1-difluoroethylene) | 268 |
Poly(trimethylene glycol) | 197 |
Poly(trimethylene terephthalate) | 328 |
Poly(vinyl acetate), PVAc, PVA | 307 |
Poly(vinyl alcohol), PVOH, PVA | 353 |
Poly(vinyl benzoate) | 344 |
Poly(vinyl butyral) | 344 |
Poly(vinyl butyrate), PVB | 278 |
Poly(vinyl chloride), PVC | 356 |
Poly(vinyl ethyl ketone) | 213 |
Poly(vinyl fluoride), PVF | 326 |
Poly(vinyl formate) | 307 |
Poly(vinyl methyl ketone) | 301 |
Poly(vinyl phenyl sulfide) | 386 |
Poly(vinyl propionate) | 283 |
Poly(vinyl stearate) | 318 |
Poly(vinylidene chloride), PVDC | 256 |
Poly(vinylidene fluoride), PVDF | 240 |
Poly(α-methylstyrene), PaMS | 445 |
Poly(ω-dodecanamide), Nylon 12 | 313 |
Poly(ω-undecanamide), Nylon 11 | 317 |